KONO 825 NGA PUKAPUKA RAraunga Raraunga

Taipitopito Hua

Tohu Hua

Whakaahuatanga Hua

Nga matotoru e waatea ana mo Alloy 825:

3/16"

1/4"

3/8"

1/2"

5/8"

3/4"

4.8mm

6.3mm

9.5mm

12.7mm

15.9mm

19mm

 

1"

1 1/4"

1 1/2"

1 3/4"

2"

 

25.4mm

31.8mm

38.1mm

44.5mm

50.8mm

 

Ko te Alloy 825 (UNS N08825) he koranu nickel-rino-chromium austenitic me nga taapiri molybdenum, parahi me te titanium. I whakawhanakehia hei whakarato i te parenga waikura tino pai i roto i nga taiao whakaheke me te whakaiti. He ātete te koranu ki te hauhautanga-waikura kapiti me te rua. Ko te taapiri o te titanium ka whakapumau i te Alloy 825 ki te whakamaarama i roto i te ahuatanga ka paiherea ka taea e te koranu te aukati ki te whakaeke i waenga i muri i te paahitanga ki te mahana i roto i te awhe ka whakapouri i nga tira kowiri kore-pumau. Ko te hanga o te Alloy 825 he ahua o nga koranu turanga nika, he mea ngawari te hanga me te weldable e nga momo tikanga.

N08367 - 1.4529 - Incoloy 926 tutaki

Pepa Whakatakotoranga

Hastelloy C4 - N06455 pereti wera wera

mo Alloy 825 (UNS N08825)

W.Nr. 2.4858:

He Kohanga Nikeli-rino-Chromium Austenitic i Whakawhanakehia mo te Atete Waihanga Tino I Roto I nga Taiao Whakakore me te Whakaiti

● Nga Taonga Whanui

● Nga tono

● Paerewa

● Tātari matū

● Āhuatanga ā-tinana

● Nga Taonga Miihini

● Atete Te Waikura

● Stress-Corrosion Kapiti Ātete

● Atete Riu

● Atete Waihanga Kawa

● Atete Waikura Intergranular

Nga Tikanga Whanui

Ko te Alloy 825 (UNS N08825) he koranu nickel-rino-chromium austenitic me nga taapiri molybdenum, parahi me te titanium. I whakawhanakehia hei whakarato i te tino parenga ki te maha o nga taiao haukino, te waikura me te whakaheke.

Ko te ihirangi nickel o Alloy 825 e kaha ana ki te chloride ahotea-waikura kapiti, me te whakakotahi ki te molybdenum me te parahi, ka tino pai ake te aukati waikura i roto i te whakaiti i nga taiao ina whakaritea ki nga tira kowiri tira austenitic. Ko te ihirangi chromium me te molybdenum o Alloy 825 e whakaahuru ana ki te rua hauhauota, tae atu ki te atete ki nga momo hau whakapouri. Ko te taapiri o te titanium ka whakapumau i te koranu ki te whakamohiotanga i roto i te ahuatanga kua paiherea. Ma tenei whakapumautanga ka taea e Alloy 825 te atete ki te whakaeke i waenga i nga kowhatu i muri i te puta ki roto i te awhe o te pāmahana e whakararu ana i nga tira kowiri kore-pumau.

Ko te Alloy 825 he ātete ki te waikura i roto i te maha o nga momo taiao tukanga tae atu ki te sulfuric, sulfurous, phosphoric, nitric, hydrofluoric me te waikawa waro me te kawakore penei i te konutai, te konutai konutai ranei, me nga otinga hauota waikawa.

Ko te hanga o te Alloy 825 he ahua o nga koranu nika-papa, me nga rawa ka taea te hanga me te weldable e nga momo tikanga.

Nga tono

● Mana Whakararurangi
● Kaihoroi
● Taputapu Tukatuka matū
● Waikawa
● Alkalis
● Taputapu Tukatuka Kai
● Nuclear
● Te Tukatuka Wahine
● Whakarewa Huānga Wahine
● Te Whakahaere Parapara
● Whakangao Hinu me te Hau
● Whakawhiti Wera Wai Moana

● Pūnaha Paipa
● Wae Hau Kawa
● Tukatuka Ore
● Taputapu Parapara Parani
● Whakapai hinu
● Nga Whakawhiti Wea Whakamaeke-rangi
● Taputapu Piki maitai
● Whakawera Coils
● Tane
● Kaata
● Kete
● Te Parapara
● Pūnaha Paipa Pai Werohanga

Paerewa

ASTM..................B 424
ASME.................SB 424

Tātari matū

Uara Angamaheni (Taumaha %)

Nickel

38.0 min.–46.0 te teitei.

Te rino

22.0 min.

Chromium

19.5 min.–23.5 te teitei.

Molybdenum

2.5 min.–3.5 te teitei.

Molybdenum

8.0 min.-10.0 te teitei.

Te parahi

1.5 min.–3.0 te teitei.

Titanium

0.6 min.–1.2 te teitei.

waro

0.05 mōrahi.

Niobium (me te Tantalum)

3.15 min.-4.15 te teitei.

Titanium

0.40

waro

0.10

konupora

1.00 te teitei.

whanariki

0.03 te teitei.

Silicon

0.5 mōrahi.

Konumohe

0.2 mōrahi.

 

 

Āhuatanga ā-tinana

Kiato
0.294 lbs/in3
8.14 g/cm3

Wera motuhake
0.105 BTU/lb-°F
440 J/kg-°K

Modulus of Elasticity
28.3 psi x 106 (100°F)
196 MPa (38°C)

Te uruhanga aukume
1.005 Oersted (μ i te 200H)

Te Whakawhitinga Ngawha
76.8 BTU/haora/ft2/ft-°F (78°F)
11.3 W/m-°K (26°C)

Awhe Whakarewa
2500 – 2550°F
1370 – 1400°C

Te Atete Hiko
678 Ohm porohita maero/ft (78°F)
1.13 μ cm (26°C)

Taurangi Rarangi o te Roha Ngaaahu
7.8 x 10-6 in / in°F (200°F)
4 m / m°C (93°F)

Nga Taonga Miihini

Nga Ahuatanga Miihini Te Pawera Ruma Tikanga, Mii Aina

Te Kaha Tuku

0.2% Offset

Tensile Mutunga

Te kaha

Te whakaroa

roto 2 in.

Te pakeke

psi (min.)

(MPa)

psi (min.)

(MPa)

% (min.)

Rockwell B

49,000

338

96,000

662

45

135-165

Ko te Alloy 825 he pai nga ahuatanga miihini mai i te cryogenic ki te pāmahana tino tiketike. Ko te mararatanga ki te mahana i runga ake i te 1000°F (540°C) ka puta he huringa ki te hangahanga moroiti ka tino heke iho te ngongo me te kaha panga. Mo tera take, kaua e whakamahia te Alloy 825 ki nga pāmahana he mea hoahoa nga taonga ngoki-whawhati. Ka taea te whakapakari i te koranu ma te mahi makariri. Ko te Alloy 825 he pai te kaha o te paanga i te pāmahana rūma, ka mau tonu te kaha ki te pāmahana tangi.

Ripanga 6 - Charpy Keyhole Impact Strength of Plate

Te pāmahana

Takotoranga

Kaha Paanga*

°F

°C

 

ft-lb

J

Rūma

Rūma

Whakapoupou

79.0

107

Rūma

Rūma

Whakawhitiwhiti

83.0

113

-110

-43

Whakapoupou

78.0

106

-110

-43

Whakawhitiwhiti

78.5

106

-320

-196

Whakapoupou

67.0

91

-320

-196

Whakawhitiwhiti

71.5

97

-423

-253

Whakapoupou

68.0

92

-423

-253

Whakawhitiwhiti

68.0

92

Te Waihanga Atete

Ko te huanga tino pai o Alloy 825 ko tona tino pai te aukati waikura. I roto i nga taiao whakahaora me te whakaiti, te koranu ka whakahē i te waikura whānui, te rua, te waikura kapiti, te waikura intergranular me te pakaru o te ahotea-waikura pūhaumāota.

Te Atete ki nga Rongoa Waikawa Whanariki taiwhanga

Kohanga

Reiti Waikura i roto i te Roopu Taiwhanga Whanaketanga Waikawa Waikawa Mire/Tau (mm/a)

10%

40%

50%

316

636 (16.2)

>1000 (>25)

>1000 (>25)

825

20 (0.5)

11 (0.28)

20 (0.5)

625

20 (0.5)

Kaore i whakamatauria

17 (0.4)

Stress-Corrosion Kapiti Ātete

Ko te nui o te nickel content o Alloy 825 he tino kaha ki te chloride ahotea-waikura kapiti. Heoi, i roto i te whakamatautau konupora konupora chloride koropuke kino rawa atu, ka pakaru te koranu i muri i te roanga o te rongo i roto i te ōrau o ngā tauira. He pai ake te mahi a Alloy 825 i nga whakamatautau taiwhanga iti ake. Ko te ripanga e whai ake nei ka whakarāpopoto i te mahinga o te koranu.

Ātete ki te Waikura Waikura Waikura Waikura

Ko te Alloy i Whakamatauria hei Tauira U-Bend

Otinga Whakamatau

Kohanga 316

SSC-6MO

Kohanga 825

Kohanga 625

42% Magnesium Chloride (Kohua)

Rahua

Whakaranuhia

Whakaranuhia

Atete

33% Lithium Chloride (Kohua)

Rahua

Atete

Atete

Atete

26% konutai pūhaumāota (Kohua)

Rahua

Atete

Atete

Atete

Whakaranuhia - Ko tetahi waahanga o nga tauira i whakamatauhia i rahua i nga haora 2000 o te whakamatautau. He tohu tenei mo te taumata teitei o te aukati.

Te Atete Riu

Ko te ihirangi chromium me te molybdenum o Alloy 825 e whakarato ana i te taumata teitei o te aukati ki te rua o te chloride. Mo konei ka taea te whakamahi i te koranu i roto i nga taiao hauota teitei penei i te wai moana. Ka taea te whakamahi i te tuatahi ki nga tono ka taea te whakaae ki etahi poka. He pai ake i nga tira kowiri tikanga penei i te 316L, engari, i roto i nga tono wai moana kaore a Alloy 825 e whakarato i nga taumata parenga rite SSC-6MO (UNS N08367) ranei Alloy 625 (UNS N06625).

Te Atete Waihanga Kohanga

Te Atete ki te Pitting Chloride me te Waikura Kawa

Kohanga

Te Pamahana o te Hunga i te Kohanga

Whakaeke Waikura* °F (°C)

316

27 (-2.5)

825

32 (0.0)

6MO

113 (45.0)

625

113 (45.0)

*Hakarite ASTM G-48, 10% Ferric Chloride

Atete Waikura Intergranular

Kohanga

Kohuatia 65% Nitric Acid ASTM

Tikanga A 262 Mahinga C

Kohuatia 65% Nitric Acid ASTM

Tikanga A 262 Mahinga B

316

34 (.85)

36 (.91)

316L

18 (.47)

26 (.66)

825

12 (.30)

1 (.03)

SSC-6MO

30 (.76)

19 (.48)

625

37 (.94)

Kaore i whakamatauria


  • Tōmua:
  • Panuku:

  • Tuhia to korero ki konei ka tukuna mai ki a matou